Fracture Characterization of Advanced 980 MPa Steels

2018-10-24 11:23:00
LUQIMENG
Original
2901
Steel Marketing Development:           Hesham Ezzat, Dave Anderson
ArcelorMittal:                                      Steve Lynes, Tim Lim
AK Steel:                                            Kavesary Raghavan
Nucor:                                                Dean Kanelos, Andy Thompson
Honda Research of Americas:           Jim Dykeman, Skye Malcolm

University of Waterloo:


Mike Worswick, Cliff Butcher
Jose Imbert-Boyd
Armin Abedini
Kenneth Cheong
Sante DiCecco
Sam Kim
Amir Zhumagulov
Taamjeed Rahmaan
Kaab Omer


Background
? Objective
? Study Materials
? Fracture Test Methodology and Results
? Component Testing
? Conclusions

Need for Grade Diversification at 980 Strength Level

? Specialized grades now exist at
the 590 and 780 MPa strength
level. (dual phase, TRIP, etc).
? Expand Grades at 980 MPa for
enhanced:
- bending
- flanging
- energy absorption


Microstructures of early DP980 not optimized for bending and edge stretch
? These property limitations restricted the application of DP980.
? Complex part shapes and features could not be formed.
? Energy absorption targets could not be meet due to fracture problems.

1. Characterize properties of various Dual Phase 980 grades selected by
Steel Marketing Development Institute (Blind Study)
2. Investigate optimized fracture testing methodology for Advanced High
Strength Steel ?  Industrial Friendly and Efficient Methods Required
3. Perform experimental axial and bend crush experiments and assess
fracture performance


Materials can generally be described as DP with fine, uniform microstructure.


1.All grades exhibited total elongation typical of 980 level material.
2.Relatively high YS/TS ratios suggested all grades favor local formability.
3.Material #2 had unique yield point elongation behavior.

1.Performance of these grades is consistent with or above current commercial products.
2.VDA bend data is of growing industrial importance as means to evaluate material.


Priority Focus Areas

1) Material characterization at large strains and strain rates
2) Efficient method to determine forming limit strains (FLD) (Global formability)
3) Characterization in tight radius bending (Local formability/fracture)
4) Establish best practices and tests for experimental fracture characterization
*Extensive numerical characterization study pursued in tandem


? Limited hardening data
available in tensile tests
? Inverse FE modeling used to
identify hardening at large
strains for fracture
? Hardening data becomes a
function of numerical model
assumptions...

? UW developed simple method to use tensile & shear test data to obtain hardening to large strain levels
? DP980 data to 60% strain!
? Not related to FE model


? Tensile characterization from 0.001 to 1000 s-1
? Scale quasi-static data obtained to large strains for strain rates
? Efficient experimental method for constitutive characterization


Physically-motivated FLD detection methods are needed



.Formability in tight-radius bending indentified as key factor in crash performance
VDA 238-100 bend test promising but only reports bend angle


Plane Strain notch provides lower bound estimate if thinning correction performed
Correction also required for plane strain dome tests

Outer diameter is in uniaxial tension and does not contact the punch
Triaxiality = 1/3 (Butcher et al., SAE, 2013, Pathak et al., JMEP, 2016; Numisheet 2016)

? Conflicting limits provided by different specimen types if thinning correction not applied

Four tests can be used to generate physically- - meaningful fracture loci
Not the product of a simulation exercise – Real material performance can be assessed

? Relatively comparable fracture loci
? Mat 2 had the lowest hardening rate, highest hole expansion and v-bend.


Sheared Edge Failure is a  Uniaxial Tensile Mode:
Use Punched Hole Expansion Tests to Obtain  Uniaxial Failure Strain with Sheared Edge

? Sled Mass: 855kg
? Sled Velocity: 25.5km/h
? Total Energy: 21kJ
? Free Crush Distance: 100mm
? Total Crush Distance: 160mm

Axial Crush Dynamic Crash Test at UW
? Sled Mass: 855kg
? Sled Velocity: 25.5km/h
? Total Energy: 21kJ
? Free Crush Distance: 115 mm
? Total Crush Distance: 135mm





Relatively Good
Performance for 3 Grades
Repeatable Energy
Absorption
Material 3 had highest
spot weld strength and
strain rate sensitivity

Efficient and Accurate Experimental Methodologies Established for Characterization
of AHSS
1. Method to experimentally obtain hardening to large strains and strain rates
2. New FLD detection algorithm: Curvature- - based
3. Optical V- - Bend developed: Ideal plane strain test
4. Four tests required to efficiently obtain fracture locus for a material
As with FLD’s,  Use 4 Industrially Friendly Tests  to Construct Fracture Locus to
Compare Material Performance  ? Accounts for Edge Condition
New model to use four tests for rapid FE model implementation  ? Next GDIS




Write a Comment
Eight plus Three =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 色精品一区二区三区 | 激情久久久久久久久久久 | 97免费观看视频 | 色婷婷在线影院 | 欧美一区二区三区免费 | 秘果电影高清完整版在线观看 | 黄视频观看 | 99热最新网址 | 精品一区二区三区视频在线观看免 | 久久精品日日躁夜夜躁欧美 | www.亚洲视频.com| 精品精品 | 奇米电影网| 天天躁日日2018躁狠狠躁 | 潦草影视在线 | 狠狠综合久久久久综 | 亚洲经典在线 | 精品视频中文字幕 | 五月婷婷综合在线视频 | 久久精品国产69国产精品亚洲 | 99精品视频免费在线观看 | 偷自视频区视频真实在线 | 国产精品一区二区久久 | 久久精品久久久久观看99水蜜桃 | 一级毛片完整免费版 | 九九精品国产兔费观看久久 | 久久国产精品一区 | 日韩成人精品在线 | 草操影院 | 青春韩国无删减版电影在线观看 | 手机看片国产免费永久 | 久久久久免费精品国产 | 激情综合网婷婷 | 四虎影院中文字幕 | 日本高清不卡网站免费 | 日本精品久久久久中文字幕2 | 日本无吗免费一二区 | 六月丁香色婷婷 | 激情五月婷婷在线 | 欧美成人短视频 | 国产成人一区 |