Detection of the Onset of Necking and Accurate Measurement of Strain Limits of AHSS

2018-10-30 16:22:00
LUQIMENG
Original
2878
Junying Min, Tongji University

John E. Carsley, General Motors Company


A neck is a groove that may develop during plastic deformation that deepens and may lead to fracture during the stamping process.

Onset of necking is defined to be the condition at a neck becomes detectable by tactile or visible sensing of the groove of the neck.


The condition of the onset of necking is important to know because localized necking is an unacceptable manufacturing condition.


The challenge is how to measure the onset of necking without having to measure 100’s of test results over a range of severity in the process of neck formation to find a few tests that are as close as possible to the condition to qualify as at the onset of a neck.


Why is this flawed?
? Result depends on the order of the polynomial.
? Shape of the strain distribution depends on the geometry of the tooling and the blank, and therefore the result of the fit with be affected by this.
? The value might be in the ballpark… it might even be a satisfactory conservative limit, but is that good enough?

Measured strains near fractured edge identified to be within the neck (beyond onset of necking)


Measured strains outside the neck

Correction for Nonlinear Strain Path

Many researchers believe that the DIC recorded strain history can be used to determine onset of necking.


Clearly the record of these strains show an increase in the strain rate as the test approaches fracture.


But strain acceleration also results from inhomogeneous straining, even if a neck does not form.


How does one de-convolute a strain signal from localized neck groove from other factors?


Selected points along the line CD that would
eventually form the neck and later fracture

Fit these points to a circle to determine the curvature





An improved curvature method of detecting the onset of localized necking
in Marciniak tests and its extension to Nakazima tests


Junying Min, Thomas B. Stoughton, John E. Carsley, Jianping Lin
International Journal of Mechanical Sciences, 2017,  123, 238-252


Challenges

Fitting to conditions near
zero curvature.


Add an artificial curve to data to avoid zero.
Solutions
Marciniak and
Nakajima test signals
are different.


Redefine Nakajima surface data to a
spherical coordinate system using radius and
arc length.


Selection of the data to
follow the groove.


A) Expand the analysis to cover the area of the
groove.


B) Adopt the approach proposed by the University of
Waterloo (Warswick, et al.).



Scale of local curvature fit is set to 1.5 times the sheet thickness 

Run the curvature fit from A to B for each frame

Let’s look at what these curvature fits look like in the LAST frame before fracture


Focus on the geometry of the DIC surface data to detect the true onset of necking.


Do not support the ad-hoc strain analyses proposed in Europe and current ISO Standards.


This focus on meaningful measurements will enable us to make wider use of AHSS’s by taking more advantage of their limited ductility through more reliable knowledge of their actual limits.


Write a Comment
Nine plus Nine =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 欧美性视频网 | 婷婷狠狠五月天小说免费 | 婷婷综合久久中文字幕蜜桃三 | 成人你懂的 | 欧美在线一级视频 | 国产一区亚洲欧美成人 | 欧美精品99 | 国产在线视频www色 国产在线视频www片 | 国产成人亚洲午夜电影 | 青草青视频在线观看 | 综合久青草视频 | www.男人天堂 | 乱老女人一二区视频 | 国产精品香蕉在线 | 日本免费专区 | 五月天婷婷视频在线观看 | 五月天丁香六月欧美综合 | 激情综合五月网 | 3344永久在线观看视频免费 | 高清国产精品久久 | 狠狠色噜噜狠狠狠狠97不卡 | 5月丁香婷婷 | 欧美激情久久久久久久久 | 国产成人亚洲精品2020 | 欧美高清日韩 | 国产成人lu在线视频 | 欧美 日韩 中文字幕 | 亚洲午夜久久久 | 国产一级在线 | 精品久久久久久中文字幕 | 欧美日本日韩 | 奇米激情网 | 国产人成亚洲第一网站在线播放 | 亚洲乱码国产乱码精品精98 | 人人干人人草 | 欧美国产精品久久 | 国产精品成人一区二区1 | 国产精品久久久久久亚洲小说 | 四虎永久在线观看免费网站网址 | 国产精品视频分类 | 欧美日韩一区二区在线视频 |